dc.description.abstract |
The work presented in this thesis shows the study of different parameters of ion beam
emanated from a conventional 2.3 kJ plasma focus device which are used for the
deposition of thin films on zirconium substrate. These energetic ions are characterized by
employing BPX65 photodiode detector placed at 9 cm along the anode axis and is used to
estimate ion energy (range from 40 keV to 1.2 MeV) and ion number density (9.7×1019 m-
3
to 1.796×1019 m-3) of the ions emitted during one focus shot. The relativistic electrons
emitted from DPF device play a vital role to incorporate the third element (ablated from
the insert material placed at the anode tip by the bombardment of relativistic electrons)
into the substrate matrix and to deposit composite films on different substrates.
The composite films are characterized by employing different characterization techniques
such as XRD, SEM, EDS, Raman Spectroscopy and Vickers microhardness tester to
explore the diverse surface properties (crystal structural, surface morphology, crystallite
size, microstructure features, elemental compositions and surface microhardness) of the
composite films. TRIM code and micro-indentation measurements are used to estimate
the depth profile of the modified layers.
Nitriding of zirconium by employing the energetic nitrogen ions emanated from plasma
focus device for multiple focus shots when the samples are placed at different angular
positions confirms the formation of zirconium nitride films on zirconium substrate. The
crystallinity and crystallite size of nitride phases increase with the increase of focus
deposition shots while residual stresses are maximum at lower nitrogen content (lower
number of focus shots) which decrease with the increase of nitrogen contents. Smooth
and uniform surface morphology showing granular features of nitrides is observed at 10o.
The nitrogen content in the deposited films increases with the increase of focus
deposition shots. The microhardness of the deposited film enhances up to 400% and
increased by increasing the nitrogen ion dose and decreases rapidly by increasing the
angular position. Hence different features of the deposited films are strongly influenced
by ion energy flux, ion number density and sample angular position.
The XRD patterns of zirconium oxynitride nanocomposite film (deposited for 40 focus
shots at different axial positions) show that the crystallinity of ZrN, Zr3N4 and ZrO2
xvii
depends on the sample axial position as well as ion energy flux. The SEM images show
the formation of compact layer at lower axial position which is due to high ion energy
flux. The nitrogen content decreases with the increase of sample angular position. The
maximum microhardness of the layers is found to be 7200 ± 12 MPa for 10 gram
imposed load. The EDS exhibits the distribution of different elements present in the
composite films.
ZrAlON composite films are deposited on zirconium substrate showing the formation of
ZrN, Al2O3 and AlN compounds. Five focus shots are sufficient to initiate the nucleation
of ZrN and Al2O3 while 10 focus shots are enough to initiate the nucleation of AlN. The
crystal growth of nitrides/oxides increases with increasing focus shots (up to 30 focus
shots) and after that re-sputtering of the previously deposited film takes place. Smooth
surface is observed for 20 focus shots at 0o angular position while net type microstructure
is obtained for 30 focus shots. Rough surface morphology is observed for 40 focus shots.
A typical microhardness value of the deposited composite films is 5255 ± 10 MPa for 10
grams imposed load which is 3.3 times the microhardness values of unexposed sample.
The microhardness values of the exposed samples increase with increasing focus shots
(up to 30 Focus shots) and decrease for 40 focus shots due to re-sputtering of the
previously deposited composite film.
Nanocrystalline zirconium carbonitride (ZrxCNy) composite films composed of ZrN,
Zr2N and Zr3N4, ZrC and Zr2CN compounds are deposited on zirconium substrate at
room temperature for multiple focus shots. The average crystallite sizes estimated for
ZrN (200) and Zr2CN (111) planes are found to vary from 10 to 20 nm. Maximum
compressive stresses (~ 3.9 GPa) in Zr2N (002) plane for 30 focus shots while maximum
tensile stresses (~ 6.5 GPa) in ZrN (200) plane for 20 focus shots are observed. Tensile
stresses in Zr2CN (111) plane are transformed to compressive one after 30 focus ion
irradiation. Raman analysis exhibits the emergence of D and G bands relating to carbides
phases during the deposition process. The SEM microstructure shows agglomerates of
size 30 to 300 nm. The Vickers microhardness values of the composite films increase
with the increase of focus shots and is found to be 5.6 ± 0.45 GPa for 10 g imposed load
which is 4.5 times that of the untreated substrate and 1.5 ± 0.11 GPa for 200 g imposed
load which is 1.3 times that of the virgin one.
Zirconium silicon nitride composite films consisting of Si3N4 and Zr3N4 compounds are
deposited on silicon substrate at room temperature through the reaction of sputtered
silicon by ion beams and ablated zirconium from the insert by using plasma focus device.
The crystallinity of Si3N4 and Zr3N4 compounds increases with increasing ion irradiation.
The crystallite size of nitride increases (from 9 ± 1 nm to 33 ± 3.5 nm) while %
microstrain values developed in the nanocomposite films decrease (from 3.65 to 0.61)
with increasing focus shots. The SEM images reveal different microstructure patterns like
granular, oval and cauliflower types of the deposited films. It is found that crystal growth
and stress relaxation inhibit the pit formations during the deposition process. The EDS
results confirm the presence of silicon, zirconium, nitrogen and oxygen in the composite
films. |
en_US |